During a routine inspection of a 110kV substation in 2023, it was found that the temperature of the A-phase contact of the ZN63A-12 vacuum circuit breaker reached 132°C (ambient temperature 34°C), and the temperature rise reached 98K, far exceeding the 65K limit specified in GB/T 1984. Disassembly inspection found that the thickness of the oxide layer of the moving and static contacts reached 0.8mm, the contact resistance rose to 320μΩ (standard value ≤25μΩ), and carbonized black spots appeared on the inner wall of the insulating tube.
Failure mechanism
-Oxide layer formation: CuCr50 contacts are eroded by arcs during long-term operation, and the surface Cr element is preferentially oxidized to form a Cr₂O₃ insulating film, resulting in an exponential increase in contact resistance (experimental data: the resistance increases 15 times when the oxide layer thickness is 0.2mm).
-Thermal runaway process: The increase in contact resistance causes Joule heat accumulation, and the oxidation rate increases by 2 times for every 10°C increase in the contact area temperature, forming a vicious cycle.
-Insulation degradation: Epoxy resin insulation tubes begin to thermally decompose above 120°C, precipitating carbonized products (containing C=O and C-H bond breakage characteristic peaks detected by FTIR), and the surface flashover voltage drops by 60%.

So how can we avoid it?
Standardized treatment measures:
1. Contact replacement: Use a laser thickness gauge to detect the contact wear (actual measurement is 3.2mm). If it exceeds the 3mm threshold specified in DL/T 596, replace it immediately. Clean the new contact with anhydrous ethanol before installation, and apply molybdenum disulfide conductive paste (thickness ≤ 0.1mm) on the contact surface
2. Circuit repair: Use pulse current method (200A/10ms) to ablate the oxide layer to reduce the circuit resistance to 18μΩ. The insulation tube is polished with 120-grit sandpaper and impregnated with 1032 insulating paint to restore the surface resistance to 5×10¹³Ω
3. Establish a prevention system: Establish a quarterly infrared temperature measurement system (temperature difference > 10K to start warning) and configure an online monitoring device to track the opening speed in real time (alarm when the fluctuation range > 0.3m/s)
Experience summary: Oxidation contact failures are highly concealed and develop rapidly. The operation and maintenance unit must strictly implement the "measurement-analysis-replacement" three-level control mechanism, combined with live detection and disassembly inspection to ensure the reliable operation of the vacuum circuit breaker.